• CN:11-2187/TH
  • ISSN:0577-6686

机械工程学报 ›› 2026, Vol. 62 ›› Issue (18): 321-329.doi: 10.3901/JME.260952

• 材料科学与工程 • 上一篇    

扫码分享

基于DIC拉伸试验的SUS304不锈钢箔尺寸效应研究

张博1,2, 范婉婉1,2, 赵金玉1,2, 赵辰辰1,2, 杨亚玉1,2, 王涛1,2   

  1. 1. 太原理工大学机械工程学院 太原 030024;
    2. 先进金属复合材料成形技术与装备教育部工程研究中心 太原 030024
  • 收稿日期:2025-11-08 修回日期:2026-06-03 发布日期:2026-11-20
  • 作者简介:张博,男,2001年出生。主要研究方向为精密极薄带成形。E-mail:zhangbo0109@link.tyut.edu.cn;王涛(通信作者),男,1985年出生,博士,教授,博士研究生导师。主要研究方向为轧制工艺与设备及金属塑性成形研究。E-mail:twang@tyut.edu.cn
  • 基金资助:
    国家自然科学基金区域联合重点(U22A20188)和国家自然科学基金青年科学基金A类(52425504)资助项目。

Investigation of Size Effects in SUS304 Stainless Steel Foil Based on DIC Tensile Testing

ZHANG Bo1,2, FAN Wanwan1,2, ZHAO Jinyu1,2, ZHAO Chenchen1,2, YANG Yayu1,2, WANG Tao1,2   

  1. 1. College of Mechanical Engineering, Taiyuan University of Technology, Taiyuan 030024;
    2. Engineering Research Center of Advanced Metal Composites Forming Technology and Equipment, Ministry of Education, Taiyuan 030024
  • Received:2025-11-08 Revised:2026-06-03 Published:2026-11-20

摘要: 由于不锈钢箔的厚度已达到微米级,厚度与晶粒尺寸比值(厚粒比,λ)变化会使其力学性能异常变化,呈现出显著的尺寸效应。以厚度20 μm的λ范围在0.7~7.2的不锈钢箔为研究对象,通过DIC单轴拉伸试验、SEM、EBSD表征以及CPFEM模拟等手段,探究了尺寸效应对不锈钢箔材力学性能和微观组织的影响机制。结果表明,随着λ降低,不锈钢箔的位错密度降低,晶粒取向的各项异性显著、孪晶比例和织构强度均提高。其主要原因在于:①晶粒自由表面占比增加,在变形过程中位错逸出程度超越了位错堆积,位错密度降低、塑性变形阻碍减小,因此,在λ >1的范围内表现为抗拉强度和屈服强度的降低以及延伸率的提高,在λ=1时延伸率达到最高;②当λ <1时,不锈钢箔的塑性变形主要依靠单晶变形,晶粒自由表面占比已达到最大,主要起几何约束作用,过高的孪晶比例和织构强度以及晶粒取向差异造成应变集中,导致不锈钢箔的延伸率降低。

关键词: 尺寸效应, SUS304不锈钢, 单层晶箔材, 晶体塑性, 微观组织, 力学性能

Abstract: When stainless steel foil thickness reaches the micrometer scale, variations in the thickness-to-grain size ratio (λ) induce anomalous mechanical properties due to pronounced size effects. Using 20 μm-thick stainless steel foil with λ spanning 0.7~7.2, the mechanisms of size effects on mechanical behavior and microstructure were investigated via DIC tensile testing, EBSD, SEM and CPFEM simulations. Results reveal that as λ decreases, dislocation density declines, while grain orientation anisotropy, twin fraction, and texture intensity increase. Key mechanisms include: ① Enhanced free surface fraction promotes dislocation escape over pile-up during deformation, reducing dislocation density and deformation resistance, leading to decreased tensile/yield strength and improved elongation for λ >1, with peak elongation at λ =1; ② At λ <1, deformation transitions to single-crystal-like behavior under geometric constraints from maximized free surfaces. Excessive twin fractions, intensified textures, and orientation disparities induce strain localization, degrading ductility.

Key words: size effect, SUS304 stainless steel, single layer grain foil, crystal plasticity, microstructure, mechanical properties